Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® Advanced N4HG7 LS BK23593 - PA9T-GF35 - BASF

Material Data Center offers the following functions for Ultramid® Advanced N4HG7 LS BK23593:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
市场与应用
汽车:燃油系统,冷却系统,进气系统(EGR),汽车电子电气,传感器,泵,燃料电池
E&E:连接器
消费品:家用电器,消费类电子产品
加工/物理特性干 / 已调节单位Test Standard
ISO数据
模塑收缩率, 平行 0.5 / * % ISO 294-4, 2577
模塑收缩率, 垂直 0.9 / * % ISO 294-4, 2577
机械性能干 / 已调节单位Test Standard
ISO数据
拉伸模量 11500 / 11500 MPa ISO 527
断裂应力 210 / 190 MPa ISO 527
断裂伸长率 2.5 / 2.3 % ISO 527
弯曲模量, 23°C 10500 / 10500 MPa ISO 178
弯曲强度 290 / 265 MPa ISO 178
无缺口简支梁冲击强度, +23°C 90 / 70 kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C 80 / - kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 10 / 8 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 9 / - kJ/m² ISO 179/1eA
热性能干 / 已调节单位Test Standard
ISO数据
熔融温度, 10°C/min 300 / * °C ISO 11357-1/-3
玻璃化转变温度, 10°C/min 120 / * °C ISO 11357-1/-2
热变形温度, 1.80 MPa 270 / * °C ISO 75-1/-2
线性热膨胀系数, 平行 17.5 / * E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 56.5 / * E-6/K ISO 11359-1/-2
厚度为h时的燃烧性 HB / * class IEC 60695-11-10
测试用试样的厚度 0.8 / * mm -
电性能干 / 已调节单位Test Standard
ISO数据
相对介电常数., 100Hz 3.8 / 3.8 - IEC 62631-2-1
介质损耗因子, 1MHz 130 / 195 E-4 IEC 62631-2-1
体积电阻率 1E16 / 1E14 Ohm*m IEC 62631-3-1
表面电阻率 * / 1E14 Ohm IEC 62631-3-2
相对漏电起痕指数 - / 600 - IEC 60112
其它性能干 / 已调节单位Test Standard
吸水性 1.9 / * % 类似ISO 62
吸湿性 0.8 / * % 类似ISO 62
密度 1420 / - kg/m³ ISO 1183
Bulk density 700 kg/m³ -
模塑测量的特殊性能干 / 已调节单位Test Standard
ISO数据
粘数 120 / * cm³/g ISO 307, 1157, 1628
试样制备条件价值单位Test Standard
ISO数据
注塑, 熔体温度 330 °C ISO 294
注塑, 模具温度 140 °C ISO 294
函数
应力-应变.  , Ultramid® Advanced N4HG7 LS BK23593 (烘干), PA9T-GF35, BASF
应力-应变.  , Ultramid® Advanced N4HG7 LS BK23593 (状况), PA9T-GF35, BASF
正割模量-应变.  , Ultramid® Advanced N4HG7 LS BK23593 (烘干), PA9T-GF35, BASF
正割模量-应变.  , Ultramid® Advanced N4HG7 LS BK23593 (状况), PA9T-GF35, BASF
拉伸模量-温度 , Ultramid® Advanced N4HG7 LS BK23593 (烘干), PA9T-GF35, BASF
拉伸模量-温度 , Ultramid® Advanced N4HG7 LS BK23593 (状况), PA9T-GF35, BASF
典型数据
加工方法
注塑, 其它挤出成型
供货形式
粒料, 黑色
特殊性能
经热稳处理的/耐热的
特征
熔体强度, 热稳定性
耐化学试剂
通用耐化学性
应用
汽车, 电子电气
地区供应
其他信息
注塑成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .05 %
Pre/Post-processing, Pre-drying, Temperature: 120 °C
Pre/Post-processing, Pre-drying, Time: 8 h

PROCESSING
injection molding, Melt temperature, range: 320 - 340 °C
injection molding, Melt temperature, recommended: 330 °C
injection molding, Mold temperature, range: 125 - 170 °C
injection molding, Mold temperature, recommended: 140 °C
injection molding, Dwell time, thermoplastics: 5 min
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com